Morphological, structural and electrical properties of Sb2Se3 films obtained by CMPO from separate sources of Sb and Se elements for solar cells
DOI:
https://doi.org/10.52304/.v23i3.264Keywords:
electrical conductivity, structure, X-ray diffraction pattern, thin films, chemical molecular beam deposition, Sb/Se, Sb2Se3Abstract
Highly crystalline Sb2Se3 films from a separate sources of Sb and Se elements at a substrate temperature of 500°С were obtained by chemical molecular beam deposition (CMBD) method. The effect of the Sb/Se composition ratio on the morphological and electrical properties of Sb2Se3 films has been studied. Based on the presented images of the scanning electron microscope and X-ray diffraction analysis, it was revealed that all films have a crystalline (orthorhombic) structure and the crystallite size is 2−3 µm. The electrical conductivity of the films measured by the Van der Paw method varies in the range 4.3×10−5 −1×102 (Ohm⋅cm)−1 depending on the composition ratio of the partial pressure of the elements Sb/Se.