Morphological properties of solid solution films Sb2(SxSe1-x)3 for solar cells
DOI:
https://doi.org/10.52304/.v26i4.574Keywords:
Sb2Se3, Sb2S3, Sb2(Sx,Se1-x)3, solid solution, scanning electron microscopy, roughnessAbstract
High-quality crystalline films of Sb2(SxSe1-x)3 solid solutions were obtained by chemical mole
cular beam epitaxy (CMBE) and vacuum thermal evaporation methods from powders of the
binary compounds Sb2S3 and Sb2Se3 on glass and glass substrates coated with a molybdenum
layer at substrate temperature 300°C.. Energy-dispersive X-ray spectroscopy confirmed that
the obtained Sb2(SxSe1-x)3 films have a composition ratio of Sb/(S+Se) close to stoichiometry,
and the distribution of all components (Sb, S, Se) in the solid solution on the surface of the
synthesized thin films is homogeneous. Scanning electron microscopy and X-ray diffraction
analysis revealed that all films have an orthorhombic structure with a predominant orientation
of (hk1), and the crystallite sizes range from 0.25 to 6 µm. An increase in the atomic concentra
tion ratio S/(S+Se) leads to a change in the shape of the crystallites. Atomic force microscopy
investigation of the films demonstrates that the root mean square roughness increases with an
increase in S/(S+Se) ratio.